Yes—if your watch cases, straps or buckles touch the skin and you sell into the EU or UK, REACH Annex XVII entry 27 applies. Nickel release from those parts must stay below 0.5 µg/cm²/week, tested to EN 1811:2023, with EN 12472:2020 wear simulation for coated finishes. A 316L grade name is not evidence of compliance: passivation, polishing, plating and sweat all change the result. Put the limit, the test method, the finish and the evidence into your RFQ before tooling starts.

What Nickel Release Means for Watch Cases

Nickel release is not nickel content. The test measures how much nickel migrates from the surface into a synthetic sweat solution over a week, per square centimetre. A case can contain 10% nickel and release very little because a stable chromium-oxide layer covers the alloy. Another case of the same grade can fail because a brushed finish, a laser mark or a contaminated polishing bath has disrupted that layer. A mill certificate cannot answer that question.

The legal limit is a rate, not a concentration: 0.5 micrograms per square centimetre per week. A post assembly for a pierced ear has a stricter 0.2 limit, but that does not apply to watch cases. Suppliers sometimes quote it by mistake—ask them to state the limit and standard in writing.

Which Watch Parts the Nickel Rule Covers

The regulation names wrist-watch cases, watch straps and tighteners explicitly. In a typical BOM that means the case middle, bezel, caseback, crown, pushers, bracelet links, clasp, strap buckle, keeper, rivets and metal spring bars that touch the skin. The caseback is obvious, but the bracelet and clasp spend as long against the wrist and rub more.

Not every metal part is in scope. Movement bridges, rotor, screws and the case interior do not normally touch the skin, so the rule does not apply. They can still fall under the SVHC rules below. Map the skin-contact parts before testing: a report covering only the case middle will not protect a bracelet or buckle. A leather strap does not remove the duty: its metal buckle, rivets and keeper are still in scope.

The Test Behind the Claim

EN 1811:2023 is the reference method for articles in direct and prolonged skin contact. A laboratory immerses the part in a defined artificial-sweat solution for seven days, analyses the leachate for nickel, and divides the mass released by the exposed area. Results are reported in µg/cm²/week against the 0.5 limit. The 2023 edition replaced the 2011 edition; new testing should use the current method.

Coated parts need an extra step. EN 12472:2020 simulates accelerated wear and corrosion before the release test, so the laboratory measures the coating after abrasion, not the pristine surface. The law requires a non-nickel coating to keep release below the limit for two years of normal use; EN 12472 is the standard way to challenge that claim quickly. A coating that passes only before wear testing is not evidence.

Two practical points cause most disputes. The test is area-based, so a small, intricately shaped part can release more per square centimetre than a flat caseback. And the laboratory needs the production finish, not a hand-polished sample. If the sample was polished for the photo shoot while the line uses a different compound, the report describes a product you are not shipping.

Why 316L, 904L and ‘Surgical Steel’ Do Not Settle the Question

316L stainless steel contains roughly 10–14% nickel, 16–18% chromium and 2–3% molybdenum. It is a sensible default: it machines well, takes a polish and resists corrosion when properly passivated. It is not nickel-free, and the grade name does not prove the finished case passes. Passivation—nitric or citric acid treatment that removes free iron and rebuilds the chromium-oxide layer—is a process step, not a property of the alloy. A case machined and polished without adequate passivation can fail even with a 316L certificate.

904L contains more nickel, typically 23–28%, with higher chromium, molybdenum and copper. It resists chloride corrosion better, which matters for dive watches and humid markets. It is not automatically better for nickel release: the nickel is held in a stable austenitic structure, and a well-passivated 904L case can pass, but the alloy is no shortcut around testing. Our comparison of 904L and 316L watch cases covers the machining and cost trade-offs.

304 stainless steel is cheaper and contains roughly 8–10.5% nickel. Its corrosion margin is narrower, especially in acidic sweat or after brushing, so it is a higher-risk choice for skin contact. Many budget cases use 304 without problems, but ‘many’ is not a report. If a supplier proposes 304, ask for finished-part release data and a corrosion test, not a grade certificate.

‘Surgical steel’ is a commercial phrase, not a regulatory grade. It usually means 316L or a similar austenitic steel, but it has no legal definition in the EU nickel rules. The same applies to ‘hypoallergenic’: there is no harmonised test or threshold behind the word. Either claim needs a finished-part report and a legal review, not a supplier’s assurance.

Where Nickel Release Actually Comes From

The substrate is only one pathway. Decorative nickel-chrome plating is the highest-risk finish because the nickel layer sits under a thin chromium topcoat; pores, scratches and wear expose it. Gold plating often uses a nickel strike for adhesion, so nickel remains in the stack though the surface looks gold. Welded joints, laser marking and rework can also disturb the passive layer or leave contamination.

Finishing consumables matter more than most buyers expect. Tumbling media, polishing compounds, wire brushes and grinding wheels previously used on nickel-bearing steel can embed contamination in a 316L part. A supplier that runs 304 and 316L on one line without segregation may produce a case that tests worse than its certificate suggests. Ask how the line separates alloys and how often the media is changed.

Wear and geometry do the rest. Bracelet links rub, clasp edges are sharp, and caseback threads trap sweat and salt. A coating that looks continuous on a flat surface may be thin or absent on an edge, in a thread or around a spring-bar hole. Test the assembled article, or at least the worst-case finished part, not a polished coupon.

REACH Is More Than One Entry: The Other Duties

Nickel sits in REACH Annex XVII, but it is not the only obligation. The candidate list of substances of very high concern (SVHC) changes twice a year. If an article contains an SVHC above 0.1% by weight, the supplier must give the recipient enough information for safe use under Article 33, and consumers can request it. Since 2021, articles on the EU market above that threshold also need a SCIP notification to ECHA. The threshold applies per article—the watch or strap as supplied—not per shipment.

Annex XVII also restricts azo colourants in leather and textiles (30 mg/kg for each listed amine) and chromium VI in leather (3 mg/kg). Those entries sit behind the strap, but they matter if you buy leather straps and sell them with the watch. Lead, cadmium and other restricted substances can appear in solders, pigments or alloys. A full materials declaration from every tier-one supplier is the practical way to see them.

Two newer duties belong in the same file. The General Product Safety Regulation (EU) 2023/988 requires an EU-based responsible person, traceability and technical documentation kept for ten years. Connected or smart watches may also fall under RoHS and WEEE. A mechanical or quartz watch is not automatically in scope, but a model with charging, Bluetooth or a battery needs a separate review. None of this is legal advice: a nickel report is one document in a compliance file, not the whole file.

How to Read a Nickel Test Report

A usable report has six things: an ISO/IEC 17025 accredited laboratory, the exact standard and year (EN 1811:2023), any pre-treatment (EN 12472:2020), a sample matching the production SKU and finish, the result in µg/cm²/week, and a clear pass/fail against 0.5. If it does not identify the finish, alloy and supplier, it is not traceable to your product.

Read the result, not just the verdict. A ‘pass’ at 0.48 is close to the limit and deserves a second look at process control. A result of 0.05 on a polished sample says little about a brushed or PVD version. Test each finish separately: polished steel, brushed steel, black PVD, gold PVD, rose-gold PVD and plated hardware. If the bracelet and case use different alloys or suppliers, test both.

There is no legal expiry date. The report is evidence about a material, finish and process at a point in time. A new plating line, polishing compound, alloy supplier or factory can invalidate it. Build those triggers into the quality agreement and keep reports with the technical file.

RFQ Clauses That Transfer the Risk

These clauses can be adapted for an RFQ or quality agreement. They are specific enough to audit but do not replace your compliance adviser’s review.

Specification point

Wording to put in the RFQ or quality agreement

Scope

Every metal part in prolonged skin contact: case, bezel, caseback, crown, pushers, bracelet, clasp, buckle, keeper and spring bars.

Limit and method

Nickel release ≤0.5 µg/cm²/week to EN 1811:2023; coated parts pre-treated to EN 12472:2020.

Base material

316L stainless steel, passivated after finishing. No 304 or unspecified steel without written approval and finished-part test evidence.

Plating

No decorative nickel or nickel-chrome plating on skin-contact surfaces. If unavoidable, specify the barrier and test after EN 12472.

Coating integrity

PVD or DLC must be continuous on all skin-contact surfaces and remain intact after EN 12472, including edges, threads and recesses.

Evidence

ISO/IEC 17025 accredited report per SKU, colour and finish before first shipment, identifying the sample and production process.

Change control

Any change of alloy supplier, plating line, polishing compound, coating supplier or heat treatment needs written notice and re-test.

Records and claims

Keep certificates and reports for at least ten years. No ‘nickel-free’ or ‘hypoallergenic’ claims without legal approval and test evidence.

Material and Finish Choices: A Practical Ranking

Use this as a starting point for the BOM conversation, then verify with finished-part testing. The ranking is about nickel-release risk, not overall quality.

Material or finish

Nickel-release risk and what to specify

Titanium (Grade 2 or 5)

No nickel in the substrate; lowest risk. Specify the grade and finish, and keep steel tooling and media separate.

Ceramic (zirconia)

No nickel; hard and scratch-resistant, but brittle at edges. Design tolerances and edge radii for ceramic.

316L stainless steel, passivated

Nickel-bearing but usually compliant when properly passivated and free of nickel plating. Test every finish.

904L stainless steel

Higher nickel (about 23–28%) but better chloride resistance. Compliance still depends on passivation and finish.

304 stainless steel

Lower cost, narrower corrosion margin. Higher risk in acidic sweat and brushed finishes; require data.

PVD or DLC over 316L

The coating can act as a barrier, but risk concentrates at edges, threads and defects. EN 12472 is essential.

Nickel-chrome decorative plating

Highest risk: the nickel underlayer is exposed by pores, scratches and wear. Avoid on skin-contact parts.

Titanium and ceramic remove nickel from the substrate but bring constraints: titanium is harder to machine and finish, and ceramic needs different tolerances and edge design. Our guide to ceramic watch cases and bezels covers the grades. With steel, the biggest gains come from eliminating nickel plating and controlling passivation, not from a more exotic alloy.

If You Sell in the UK, US or Elsewhere

The UK retained the same 0.5 µg/cm²/week limit after Brexit, through UK REACH and the national nickel safety regulations. The test method is familiar; the responsible operator and import paperwork are different. If you ship to both markets, build one test file that satisfies both and keep the importer details separate.

The US has no federal nickel-release limit equivalent to REACH. Claims fall under the FTC’s jewellery guides, and California’s Proposition 65 can require warnings for listed chemicals above threshold. Some retailers impose stricter specifications. Canada, Japan and the Gulf have different regimes. Adopt the EU limit as your global default: it is the benchmark most serious suppliers know.

A Six-Step Pre-Launch Workflow

  • Step 1 — Map the skin-contact parts: every metal component touching the wrist, including bracelet, clasp, buckle, crown and caseback.

  • Step 2 — Choose material and finish. Eliminate nickel plating first, then compare 316L, 904L, titanium or ceramic on design and cost.

  • Step 3 — Write the requirement into the RFQ: limit, standards, sample identity and change-control trigger.

  • Step 4 — Test the worst case: each production finish, with EN 12472 pre-treatment for coated parts, at an accredited laboratory.

  • Step 5 — Review the whole file: the report, the SVHC and SCIP position, and the GPSR technical documentation.

  • Step 6 — Lock the process: record the approved alloy, finish, plating line and report; re-test after any change.

FAQ

Does 316L stainless steel pass the EU nickel test?

Not automatically. 316L contains roughly 10–14% nickel. A correctly passivated, polished case often passes, but cast, brushed, laser-marked or contaminated parts can fail. Test the finished part.

Is 904L better for nickel allergy?

Not necessarily. 904L contains more nickel; its advantage is chloride corrosion resistance. Release depends on the passive layer and finish, so it still needs a finished-part report.

Can PVD or DLC coating make a nickel-containing case compliant?

A continuous, defect-free coating can reduce release, but the law tests the coated article after EN 12472 wear. Edges, threads and pores are the failure points. Do not rely on a coating without a report.

Do watch straps and buckles need nickel testing?

Metal buckles, clasps, rivets and keepers that touch the skin are in scope. Leather has separate azo dye and chromium VI limits. Test the metal hardware as fitted.

How long does a nickel test report last?

There is no legal expiry. A report is tied to a material, finish and process. Re-test after any change; many brands require annual verification or a report per lot.

Does REACH apply if my brand is outside the EU?

Yes, if the product is placed on the EU market. The importer or fulfilment provider may be the responsible operator, but the brand still needs the evidence. UK sales need UK REACH.

Compliance is a specification, not a certificate. A nickel report is a snapshot of one finish on one day; the brands that stay out of trouble control the alloy, passivation, plating and change process around it. Put the requirement in the RFQ, make the test a pre-production gate, and keep the evidence on file. Our OEM watch manufacturer checklist covers the questions to ask before tooling, and our guide to watch case manufacturing explains where polishing and passivation sit.

Comments


© Copyright
  • Ching Chi Instagram
  • Ching Chi facebook
  • Whatsapp to Ching Chi
  • Ching Chi's LinkedIn

+852 2499 8113

Unit 12,17/F., Cheung Fung Industrial Building, 23-29 Pak Tin Par Street, Tsuen Wan, N.T., Hong Kong.

©2026 by Ching Chi Industrial Co. Ltd

​

Hong Kong Branch Certificate for Category A Registrant (Section 53ZUG, Cap 615) : A-B-24-01-05227

Ching Chi Industrial Co. Ltd, Dun & Bradstreet Business Verified
bottom of page